Technical Guide

Inconel 706: Precipitation-Hardening Superalloy for Large Turbine Components

UNS N07706 / W.Nr. 2.4662 — Cost-effective nickel-iron-chromium superalloy with outstanding tensile strength, excellent fabricability, and proven performance in large gas turbine discs and shafts.

Inconel 706 alloy forged disc and bar for large gas turbine components - Shanghai Hangbo Alloy
← Back to Knowledge Center

What is Inconel 706?

Inconel 706 (UNS N07706 / W.Nr. 2.4662) is a precipitation-hardenable nickel-iron-chromium superalloy that shares a close metallurgical lineage with the widely used Inconel 718. Developed by Special Metals Corporation as a more cost-effective alternative for large structural components, Inconel 706 offers comparable mechanical strength and fabricability while using significantly less nickel — approximately 39–44% versus 50–55% in Inconel 718. The higher iron content (28–35%) reduces raw material costs without sacrificing the essential gamma double-prime (Ni3Nb) strengthening mechanism that provides the alloy’s high tensile and yield properties.

The primary engineering rationale for Inconel 706 lies in its superior hot-working characteristics for large section sizes. When forging gas turbine discs exceeding 600 mm in diameter, Inconel 718 can develop harmful grain-boundary precipitation and structural inconsistency in the center of thick sections. Inconel 706’s modified chemistry provides improved hot ductility and more uniform grain structure throughout large forgings, making it the preferred choice for heavy rotating components in industrial gas turbines and power generation equipment.

Like Inconel 718, the strengthening of Inconel 706 relies on the precipitation of gamma double-prime (Ni3Nb) and gamma-prime (Ni3(Al,Ti)) phases during a controlled two-step aging heat treatment. The alloy’s sluggish precipitation kinetics — a direct consequence of its niobium and titanium content — allow welding and forming in the annealed condition without the risk of strain-age cracking that plagues many other precipitation-hardened superalloys. This property is critical for fabricating complex turbine assemblies that require post-weld heat treatment.

Inconel 706 is melted using vacuum induction melting (VIM) followed by vacuum arc remelting (VAR) or electroslag remelting (ESR) to ensure the cleanliness and microstructural consistency demanded by turbine specifications. The alloy is supplied in solution-annealed and aged conditions per ASTM B670 and AMS specifications. At Hangbo Alloy Group, we produce Inconel 706 round bars, large forgings, plates, and welding wire for turbine manufacturers and power generation OEMs worldwide.

Quick Specifications

N07706
2.4662
8.05 g/cm3
1260 - 1327 °C (2300 - 2420 °F)
1240 MPa (180 ksi)
1035 MPa (150 ksi)
650 °C (1200 °F)
12 - 18%

What is the chemical composition of Inconel 706?

The chemistry of Inconel 706 is deliberately positioned between Inconel 718 and the iron-nickel superalloy family. Nickel is reduced to 39–44% (compared to 50–55% in 718), while iron is raised to 28–35%, making the alloy substantially more economical. The critical strengthening elements — niobium, titanium, and aluminum — are maintained at levels that ensure robust gamma double-prime and gamma-prime precipitation during aging, though niobium is slightly lower than in 718. Carbon, sulfur, and phosphorus are tightly restricted to protect ductility and creep-rupture life in large forgings.

ElementMin %Max %
Nickel (Ni)39.044.0
Chromium (Cr)14.517.5
Iron (Fe)28.035.0
Niobium + Tantalum (Nb+Ta)2.753.75
Titanium (Ti)1.502.00
Aluminum (Al)0.200.60
Molybdenum (Mo)0.501.50
Cobalt (Co)—1.00
Carbon (C)—0.06
Manganese (Mn)—0.35
Silicon (Si)—0.35
Phosphorus (P)—0.015
Sulfur (S)—0.015
Boron (B)—0.006
Copper (Cu)—0.30

What are the physical properties of Inconel 706?

Inconel 706 has an FCC austenitic matrix in the solution-annealed condition, identical to Inconel 718. Its density of 8.05 g/cm³ is slightly lower than Inconel 718 (8.19 g/cm³) due to the higher iron content. The alloy maintains moderate thermal conductivity and a relatively low coefficient of thermal expansion, which helps minimize thermal fatigue in large rotating components that experience temperature gradients during startup and shutdown cycles.

PropertyValueUnit
Density8.05g/cm3
Melting Range1260 - 1327°C
Specific Heat (21°C)435J/kg·K
Thermal Conductivity (21°C)12.1W/m·K
Electrical Resistivity (21°C)1.20μΩ·m
Modulus of Elasticity (21°C)200GPa
Mean CTE (21-93°C)13.3μm/m·°C
Curie Temperature-196°C

What are the room-temperature mechanical properties of Inconel 706?

The mechanical properties of Inconel 706 are comparable to Inconel 718 in the aged condition, with tensile strength typically reaching 1240 MPa and yield strength 1035 MPa. These values are achieved through the standard two-step aging treatment that precipitates gamma double-prime and gamma-prime strengthening phases. The alloy retains adequate ductility (12–18% elongation) for structural reliability in turbine components. Values below are typical for bars and forgings per ASTM B670 in the aged condition.

PropertyValue
Tensile Strength1240 MPa (180 ksi)
Yield Strength (0.2% offset)1035 MPa (150 ksi)
Elongation in 2 inches12 - 18%
Reduction of Area15 - 30%
Hardness36 - 44 HRC
Charpy V-notch Impact (room temp)25 - 45 J

What are the heat treatment conditions for Inconel 706?

Inconel 706 is supplied in either solution-treated or solution-treated plus aged condition. The heat treatment schedules are essentially identical to those used for Inconel 718, reflecting the alloys’ shared strengthening mechanism. Two primary schedules are used:

  • Standard Two-Step Aging (ASTM B670): Solution anneal 954–982°C, air cool; age 718°C for 8 hours, furnace cool to 621°C and hold 8 hours, air cool. Produces tensile strength ≥1240 MPa and yield strength ≥1035 MPa.
  • Simplified Single-Step Aging: Used for large turbine disc forgings where thermal cycle complexity must be minimized. Solution anneal 954–982°C, air cool; age 718°C for 8 hours, air cool. Achieves slightly lower yield strength (~965–1000 MPa) but more uniform properties across thick sections.
  • Annealed Only: Solution anneal 1066°C for optimum formability and weldability; used when subsequent fabrication and final aging will be performed by the end user.

For large forgings, controlled cooling rates and furnace atmosphere are critical to avoid differential thermal stresses that could cause distortion or cracking in massive components. Hangbo Alloy Group provides full heat treatment certification with each order, including recorded time-temperature profiles and mechanical test results.

What are the high-temperature mechanical properties of Inconel 706?

Inconel 706 retains significant strength at elevated temperatures thanks to its gamma double-prime strengthening phase, though its high-temperature capability is slightly below Inconel 718 due to the lower niobium and nickel content. The alloy is designed for long-term service at temperatures up to approximately 650°C (1200°F). Above this temperature, the gamma double-prime precipitates begin to coarsen and transform to the equilibrium delta phase, resulting in gradual strength loss. For short-term exposure, temperatures up to 700°C are tolerable, but sustained operation above 650°C is not recommended for critical rotating components.

Temperature (°C)Tensile Strength (MPa)Yield Strength (MPa)Elongation (%)
21 (Room)1240103516
316116095017
427110092017
538103088018
64986075020
70466058026
76045038032
81628024040

How corrosion resistant is Inconel 706?

Inconel 706 provides corrosion resistance comparable to Inconel 718, which is adequate for many industrial environments though not equivalent to dedicated corrosion-resistant alloys like Hastelloy C-276 or Inconel 625. The chromium content (14.5–17.5%) provides a protective oxide scale in oxidizing atmospheres, while molybdenum and niobium contribute to resistance against chloride-induced pitting.

Resistance to Specific Media:

  • Oxidation Resistance: Forms a continuous chromium oxide scale and resists oxidation in air and combustion gases up to approximately 650°C. Above this temperature, oxide spallation increases and internal oxidation may develop.
  • Chloride Pitting and Crevice Corrosion: Good resistance to chloride pitting in marine and industrial environments, superior to standard stainless steels but less than super-austenitic or nickel-molybdenum alloys.
  • Sour Gas (H2S) Service: Suitable for oil and gas applications where hydrogen sulfide is present, provided hardness is controlled below 40 HRC per NACE MR0175 / ISO 15156.
  • Neutral and Alkaline Environments: Resistant to many neutral salt solutions and caustic environments at moderate temperatures.

Where is Inconel 706 used?

Inconel 706 was specifically developed for large structural and rotating components in gas turbines where cost-effectiveness and uniform mechanical properties through thick sections are paramount. Its lower nickel content reduces material cost by 15–20% compared to Inconel 718, while its improved hot-working behavior ensures more consistent grain structure in large forgings.

  • Industrial Gas Turbines: Large compressor and turbine discs, shafts, and casings for heavy-duty industrial gas turbines used in power generation and mechanical drive applications. This is the alloy’s primary market.
  • Power Generation: Rotors, discs, and structural bolting for combined-cycle and simple-cycle gas turbine power plants operating at temperatures below 650°C.
  • Aerospace: Secondary structural components, casings, and non-critical rotating parts where the cost advantage over Inconel 718 is significant and temperature requirements are moderate.
  • Oil and Gas: Downhole tool components and wellhead hardware where high strength and sour gas resistance are required at moderate temperatures.
  • Nuclear Power: Structural supports and bolting in reactor systems where reliable mechanical properties and corrosion resistance in high-temperature water environments are needed.

Which product forms are available for Inconel 706?

Hangbo Alloy Group manufactures and supplies Inconel 706 in a comprehensive range of product forms, all supported by material test reports and third-party inspection. Our production capacity is optimized for the large-section forgings that define this alloy’s primary market:

  • Round Bars: ASTM B670, diameters 6 mm to 350 mm, hot-rolled, forged, or cold-drawn, solution annealed or aged.
  • Forgings: ASTM B670, custom open-die and ring-rolled forgings up to 1000 mm diameter, heat treated to specification, with ultrasonic testing available per ASTM E2375.
  • Plates & Sheets: Thickness 0.5 mm to 50 mm, solution annealed or aged, for fabrications and structural components.
  • Welding Wire: AWS A5.14 ERNiFeCr-2, precision layer-wound, for repair and fabrication of Inconel 706 and 718 components.

Which standards cover Inconel 706?

StandardDescription
ASTM B670Bar, Forging, and Forging Stock, Precipitation Hardened
AMS 5680Wire, Solution Treated
AMS 5681Wire, Precipitation Hardened
AWS A5.14Welding Wire (ERNiFeCr-2)
ASME SB-670Boiler and Pressure Vessel Code
NACE MR0175 / ISO 15156Sour Gas Service (Hardness ≤40 HRC)

General references: Nickel Institute · AMPP · SAE International · ASTM International

Frequently Asked Questions (FAQ)

What is the density of Inconel 706?

Inconel 706 has a density of 8.05 g/cm³ (0.291 lb/in³), slightly lower than Inconel 718 (8.19 g/cm³) due to its higher iron content (~40% vs balance). This lower density can reduce the weight of large turbine discs by approximately 1.7%.

What is the melting point of Inconel 706?

The melting range of Inconel 706 is approximately 1260–1327°C (2300–2420°F), comparable to Inconel 718’s range of 1260–1336°C.

What is the chemical composition of Inconel 706?

Inconel 706 (UNS N07706) nominal composition: Ni 39–44%, Cr 14.5–17.5%, Fe 28–35%, Nb+Ta 2.75–3.75%, Ti 1.5–2.0%, Al 0.2–0.6%, Mo 0.5–1.5%, C ≤0.06%, Mn ≤0.35%, Si ≤0.35%, S ≤0.015%, P ≤0.015%, B ≤0.006%. Key difference from 718: higher iron, lower nickel, slightly lower niobium.

What standards apply to Inconel 706?

Key standards for Inconel 706 include ASTM B670 (bar and forging), AMS 5680 (wire), AMS 5681 (wire, precipitation hardened), and ASME SB-670 for pressure vessel applications. NACE MR0175 / ISO 15156 applies for sour gas service with hardness control.

What is the heat treatment for Inconel 706?

The standard two-step aging for Inconel 706 is: solution anneal at 954–982°C, air cool; age at 718°C for 8 hours, furnace cool to 621°C, hold 8 hours, then air cool. A single-step aging (718°C/8h/AC) is also used for larger forgings requiring simplified thermal cycles, achieving slightly lower but more uniform properties across thick sections.

How does Inconel 706 compare to Inconel 718?

Inconel 706 is derived from Inconel 718 with higher iron (28–35% vs balance) and lower nickel (39–44% vs 50–55%). This makes 706 more cost-effective while maintaining similar mechanical properties. 706 has comparable yield strength (~1035 MPa) and tensile strength (~1240 MPa) but slightly lower creep resistance above 650°C. Its main advantage is easier hot working for large forgings and 15–20% lower material cost.

What is the price range for Inconel 706?

Inconel 706 is typically 15–20% less expensive than Inconel 718 due to its higher iron content (lower nickel consumption). Rough price range: $18–30/kg for round bar in standard sizes, depending on form, size, and specification. Large custom forgings may have higher per-kg costs due to processing complexity. Contact Hangbo Alloy Group for current pricing and availability.

What product forms are available for Inconel 706?

Inconel 706 is available as round bars (6–350 mm dia), forgings (custom open-die and ring-rolled up to 1000 mm diameter), plates and sheets (0.5–50 mm), and welding wire (ERNiFeCr-2 / AWS A5.14). Hangbo Alloy Group supplies all forms per ASTM B670 and AMS specifications with full certification.

Is Inconel 706 weldable?

Yes, Inconel 706 has excellent weldability similar to Inconel 718. It can be welded by GTAW (gas tungsten arc), GMAW (gas metal arc), and EBW (electron beam) using matching filler metal ERNiFeCr-2. Its sluggish precipitation kinetics prevent strain-age cracking during post-weld heat treatment, a critical advantage for fabricating complex turbine assemblies.

What is the maximum service temperature of Inconel 706?

Inconel 706 is designed for service up to approximately 650°C (1200°F) for long-term applications. Short-term exposure to 700°C is possible, but above 650°C the gamma double-prime precipitates begin coarsening, causing gradual strength loss. For critical rotating components, 650°C is the recommended maximum continuous service temperature.

What are typical lead time and MOQ for Inconel 706?

Standard round bars (ASTM B670): typical lead time 15–25 days, MOQ 100 kg. Custom forgings for turbine discs: lead time 45–90 days depending on size and specification, MOQ negotiable. Welding wire: 10–15 days, MOQ 50 kg. Hangbo Alloy Group maintains stock of common bar sizes for rapid delivery.

Contact Us for Inconel 706

Hangbo Alloy Group maintains mill-direct supply of Inconel 706 round bars, large forgings, plates, and welding wire in both solution-treated and aged conditions per ASTM B670. Our team specializes in large-section turbine disc forgings and can assist with material selection, heat treatment specification, ultrasonic testing requirements, and export documentation.

For quotations, material certifications, or technical consultation, contact our sales team or call +86 13611656360. We typically respond within 10 minutes.

Need Inconel 706 Material?

Request a quotation for Inconel 706 round bars, turbine disc forgings, plates, or welding wire. We supply standard sizes and accept custom forging orders up to 1000 mm diameter.