Technical Guide

Nimonic 105: High-Temperature Superalloy & Gas Turbine Blade Applications

UNS N07112 — Nickel-cobalt-chromium precipitation-hardened superalloy with high gamma prime volume fraction, outstanding creep-rupture strength at 800–900 °C, and gas turbine blade and disc applications.

Nimonic 105 nickel-based precipitation-hardened superalloy forged bar and turbine blade material - Shanghai Hangbo Alloy
← Back to Knowledge Center

What is Nimonic 105?

Nimonic 105 (UNS N07112) is a high-performance nickel-cobalt-chromium precipitation-hardened superalloy developed by Special Metals Corporation (originally Henry Wiggin & Company) for gas turbine blade and disc applications operating at temperatures up to 900 °C. It belongs to the Nimonic family of alloys, which were among the first purpose-designed superalloys for the British jet engine industry in the 1940s–1960s, and Nimonic 105 represents the highest-strength forged variant in the series.

The defining feature of Nimonic 105 is its exceptionally high combined aluminum-plus-titanium content (~9%), which produces a gamma prime (Ni3(Al,Ti)) volume fraction of approximately 45% after the full four-step heat treatment. This is significantly higher than Nimonic 80A (~30%), Nimonic 90 (~30%), or Inconel 718 (~30%), and it is the principal source of the alloy’s outstanding creep-rupture strength at temperatures where the gamma prime phase is still stable. Cobalt (~15%) provides additional solid-solution strengthening and stabilizes the gamma prime phase against dissolution at elevated temperature, while chromium (~15%) provides oxidation resistance and molybdenum (~5%) adds further solid-solution strength.

Nimonic 105 was developed as an evolution of Nimonic 90, with aluminum raised from ~2% to ~5% and titanium from ~2.5% to ~4%, plus molybdenum added at ~5%. These changes doubled the gamma prime volume fraction and dramatically improved creep-rupture life at 800–900 °C, making Nimonic 105 suitable for the highest-stress, highest-temperature forged blade and disc positions in both aero and industrial gas turbines. The trade-off was significantly reduced weldability and a more complex heat treatment sequence.

At Hangbo Alloy Group, Nimonic 105 is melted by vacuum induction melting (VIM) followed by vacuum arc remelting (VAR) for the cleanest possible ingot structure, then forged and solution-treated. Each lot is tested for chemical composition, grain structure (ASTM grain size 3–5 for creep-optimized forging), tensile properties, and creep-rupture life per OEM specifications.

Quick Specifications

N07112
—
8.01 g/cm³
1315–1370 °C
1100–1200 MPa
750–850 MPa
~45%
10–15%
~900 °C (peak)
Excellent

What is the chemical composition of Nimonic 105?

The composition of Nimonic 105 is optimized for maximum gamma prime volume fraction while maintaining sufficient chromium for oxidation resistance and cobalt for gamma prime stability. The combined Al+Ti content of ~9% is the highest among the commonly forged Nimonic alloys and is the principal driver of the alloy’s exceptional creep-rupture strength. The carbon and boron additions provide grain-boundary strengthening through carbide and boride precipitation, while zirconium helps control grain-boundary morphology during long-term creep exposure.

ElementMin %Max %
Nickel (Ni)Balance (~53)Balance
Cobalt (Co)14.017.0
Chromium (Cr)14.515.5
Aluminum (Al)4.55.0
Titanium (Ti)3.74.2
Molybdenum (Mo)4.55.0
Carbon (C)0.120.17
Boron (B)0.0030.008
Zirconium (Zr)0.050.15
Iron (Fe)—1.0
Manganese (Mn)—0.25
Silicon (Si)—0.25
Sulfur (S)—0.015
Lead (Pb)—0.005
Silver (Ag)—0.0005
Bismuth (Bi)—0.0001

What are the physical properties of Nimonic 105?

Nimonic 105 has an austenitic (FCC) matrix structure at all service temperatures, with approximately 45% of the volume occupied by gamma prime (Ni3(Al,Ti)) precipitate particles after the full heat treatment. The gamma prime particles are coherent with the matrix and provide the primary strengthening mechanism. Their size and distribution are controlled by the four-step heat treatment: the first aging at 1065 °C precipitates the primary coarse gamma prime, while subsequent lower-temperature aging steps precipitate finer secondary gamma prime particles between the coarse ones, creating a dual-size distribution that maximizes both short-time strength and long-time creep resistance.

PropertyValueUnit
Density8.01g/cm³
Melting Range1315–1370°C
Specific Heat (20–100 °C)~450J/kg·K
Thermal Conductivity (20 °C)~11.5W/m·K
Electrical Resistivity (20 °C)~1.19μΩ·m
Modulus of Elasticity (20 °C)~225GPa
Mean CTE (20–100 °C)~11.5× 10−6/°C
Mean CTE (20–500 °C)~13.0× 10−6/°C
Mean CTE (20–800 °C)~14.5× 10−6/°C
Mean CTE (20–900 °C)~15.5× 10−6/°C

What are the mechanical properties of Nimonic 105?

Nimonic 105 achieves its mechanical properties through the full four-step heat treatment, which produces the optimal dual-size gamma prime distribution and a controlled grain size (typically ASTM 3–5 for creep-optimized material). Room-temperature strength is very high due to the ~45% gamma prime volume fraction, but the alloy’s primary value lies in its elevated-temperature strength and creep-rupture performance, which far exceed those of Nimonic 80A, Nimonic 90, or Inconel 718 at temperatures above 800 °C.

PropertySolution TreatedFully Aged (4-step)
Tensile Strength~700 MPa (102 ksi)1100–1200 MPa (160–175 ksi)
Yield Strength (0.2%)~350 MPa (51 ksi)750–850 MPa (110–125 ksi)
Elongation (in 50 mm)~40%10–15%
Hardness~25 HRC36–40 HRC
Reduction of Area~50%12–18%

What are the high-temperature mechanical properties of Nimonic 105?

The high-temperature strength of Nimonic 105 is its defining engineering advantage. At 800 °C, tensile strength remains above 600 MPa, and the creep-rupture life at 800–870 °C under moderate stress (150–200 MPa) exceeds that of all earlier Nimonic alloys by a substantial margin. This is directly attributable to the high gamma prime volume fraction, which remains stable at these temperatures and resists dislocation climb and creep deformation.

Nimonic 105 also has good fatigue resistance at elevated temperature, particularly in the low-cycle fatigue regime relevant to turbine disc applications where cyclic thermal and centrifugal stresses combine. The controlled grain size (ASTM 3–5) and dual-size gamma prime distribution provide a balance between creep resistance (favoring coarser grains) and fatigue resistance (favoring finer grains).

Temperature (°C)Tensile Strength (MPa)Yield Strength (MPa)Elongation (%)
20 (RT)1100–1200750–85010–15
600950–1050650–75012–18
700800–900500–60015–20
800600–700350–45018–25
870450–550250–35020–30
900350–450180–28025–35

Creep-Rupture Data (Typical)

Temperature (°C)Stress (MPa)Rupture Life (hours)
800350~50
800250~300
800150>1000
870250~30
870150~200
870100>500
900150~25
900100~100

How corrosion resistant is Nimonic 105?

Nimonic 105 has good oxidation resistance at elevated temperature due to its 15% chromium content, which forms a Cr2O3 protective oxide scale. The addition of 5% aluminum further enhances oxidation resistance by forming an Al2O3 sub-scale beneath the chromium oxide. This dual-oxide system provides reasonably good protection up to 900 °C in clean combustion gas atmospheres.

However, Nimonic 105 is not a corrosion-resistant alloy in the sense of Hastelloy or Inconel 625. It is designed for high-temperature structural service in relatively clean gas turbine environments, not for chemical processing or seawater exposure.

  • Oxidation (dry air): Good up to 900 °C. The Cr+Al dual oxide system provides protection. Scale spallation begins above ~950 °C in cyclic conditions.
  • Hot corrosion (type I, Na2SO4): Moderate resistance at 800–900 °C. Aluminide or MCrAlY overlay coating is recommended for marine gas turbine service where sulfate deposits are expected.
  • Hot corrosion (type II, low-temp): Limited resistance at 600–750 °C where pitting-type corrosion predominates. Coating required.
  • Seawater: Not designed for immersion. The 15% Cr provides only moderate resistance. Avoid prolonged wet exposure.
  • Acids: Not suitable for chemical process environments. The alloy’s corrosion resistance is optimized for gas turbine combustion atmospheres, not aggressive acid media.

How is Nimonic 105 heat treated?

Nimonic 105 requires a four-step heat treatment sequence that is more complex than most other superalloys. This sequence is designed to produce the optimal dual-size gamma prime distribution and grain structure for maximum creep-rupture strength. Simplifying the heat treatment by combining or eliminating steps will reduce both short-time and long-time high-temperature properties.

  • Solution treatment: 1150 °C (2100 °F) for 4 hours, air cool. Dissolves all existing gamma prime and carbides, producing a coarse grain structure (ASTM 3–5) optimized for creep resistance.
  • First aging: 1065 °C (1950 °F) for 16 hours, air cool. Precipitates coarse primary gamma prime particles that provide the skeleton structure for creep resistance.
  • Second aging: 980 °C (1800 °F) for 16 hours, air cool. Precipitates intermediate-size gamma prime between the coarse particles, increasing short-time yield and tensile strength.
  • Third aging: 795 °C (1460 °F) for 16 hours, air cool. Precipitates fine secondary gamma prime in the matrix channels between the coarse and intermediate particles, maximizing both short-time strength and long-time creep resistance.

The 16-hour hold times at each aging step are essential for complete precipitation and uniform distribution. Shorter holds will under-age the alloy and reduce both tensile strength and creep-rupture life. The total heat treatment cycle requires approximately 80–90 hours (4+16+16+16 hours plus heating and cooling transitions), making it one of the longest and most expensive heat treatment sequences in the superalloy industry.

Where is Nimonic 105 used?

Nimonic 105 is used almost exclusively in gas turbine and aerospace applications where its combination of high gamma prime volume fraction, excellent creep-rupture strength at 800–900 °C, and good oxidation resistance makes it the optimal forged superalloy choice. It was historically a key material in British-designed gas turbines and remains in service in both aero and industrial engines worldwide.

  • Gas Turbine Blades: HP (high-pressure) and IP (intermediate-pressure) turbine blades in aero engines (Rolls-Royce Spey, Dart, Tyne) and industrial gas turbines operating at 800–900 °C. Nimonic 105 provides the highest forged-blade creep-rupture strength in the Nimonic family.
  • Turbine Discs: HP compressor and turbine discs where the combination of elevated-temperature strength, good LCF (low-cycle fatigue) resistance, and controlled grain size provides safe, reliable operation under cyclic thermal and centrifugal loading.
  • Shafts and Spacers: Turbine shaft sections and spacers that experience both torsional stress and thermal exposure.
  • Aerospace Fasteners: High-temperature bolts and studs for engine assembly where strength at 600–800 °C is required. Nimonic 105 fasteners retain preload better than Inconel 718 fasteners at temperatures above 650 °C.
  • Industrial Gas Turbine Components: Hot-section forged components in power generation and mechanical-drive gas turbines operating at 800–900 °C.
  • Forged Rings and Cases: Limited use in ring forgings for turbine case reinforcement where creep resistance at moderate stress levels is required.

Which product forms are available for Nimonic 105?

Hangbo Alloy Group supplies Nimonic 105 in the following forms, all VIM+VAR melted and solution-treated for customer-side aging:

  • Round Bars: 6–200 mm diameter, solution-treated at 1150 °C, with grain size verification. Supplied per Rolls-Royce MSRR or customer OEM specification.
  • Forging Stock and Custom Forgings: Billets and closed-die forgings per customer drawing (turbine discs, blade stock, shafts). Full mechanical testing and metallographic inspection on each forging.
  • Billets: VIM+VAR melted billets for customer-side forging, 150–350 mm diameter.
  • Wire: Limited sizes (0.5–5.0 mm) for spring and fastener fabrication.
  • Sheet/Plate: Limited availability up to 20 mm thickness for structural components.

Which standards cover Nimonic 105?

StandardDescription
MSRR 7012Rolls-Royce Material Specification for Nimonic 105 Bar
MSRR 7013Rolls-Royce Specification for Nimonic 105 Forgings
MSRR 7014Rolls-Royce Specification for Nimonic 105 Sheet
BS HR3British Standard for Nimonic 105
GE Spec (various)GE Aviation Specifications for Nimonic 105 Components
SAE AMS 2269Chemical Check Analysis Limits for Nickel Alloys

General references: Nickel Institute · AMPP · SAE International · ASTM International

Frequently Asked Questions (FAQ)

Q1. What is Nimonic 105?

Nimonic 105 (UNS N07112) is a nickel-cobalt-chromium precipitation-hardened superalloy with ~9% combined Al+Ti, producing ~45% gamma prime volume fraction and outstanding creep-rupture strength at 800–900 °C. It was developed for gas turbine blade and disc applications and is the highest-strength forged alloy in the Nimonic family.

Q2. What is the chemical composition of Nimonic 105?

Ni balance (~53%), Co 14–17%, Cr 14.5–15.5%, Al 4.5–5.0%, Ti 3.7–4.2%, Mo 4.5–5.0%, C 0.12–0.17%, B 0.003–0.008%, Zr 0.05–0.15%, Fe ≤1.0%. The high Al+Ti content (~9%) drives the large gamma prime fraction.

Q3. What is the density of Nimonic 105?

Density is 8.01 g/cm³. Melting range is 1315–1370 °C. Gamma prime volume fraction is ~45% after full heat treatment. Grain size is typically ASTM 3–5 for creep-optimized forging.

Q4. What standards cover Nimonic 105?

Nimonic 105 is covered by Rolls-Royce MSRR 7012 (bar), 7013 (forging), 7014 (sheet), British Standard BS HR3, and various GE Aviation specifications. There is no direct ASTM specification; it is typically ordered per OEM proprietary specs.

Q5. What is the tensile strength of Nimonic 105?

After the four-step heat treatment, Nimonic 105 achieves RT tensile strength of 1100–1200 MPa and yield strength of 750–850 MPa, with elongation 10–15%. At 800 °C, tensile strength remains above 600 MPa.

Q6. How does Nimonic 105 compare to Nimonic 90?

Nimonic 105 has significantly higher creep-rupture strength at 800–900 °C due to ~45% gamma prime (vs ~30% in Nimonic 90). Key composition differences: Al 5% vs 2%, Ti 4% vs 2.5%, Mo 5% vs 0%. Nimonic 105 also has higher cobalt (15% vs 20% in Nimonic 90). Nimonic 90 is better for applications below 800 °C where weldability is needed.

Q7. What is the maximum service temperature of Nimonic 105?

Nimonic 105 is designed for service up to 900 °C for short-duration peak conditions and 870 °C for long-term continuous creep-rupture service. Above 950 °C, gamma prime dissolution and oxidation become limiting. Coating (aluminide or MCrAlY) extends the oxidation-safe limit.

Q8. What is the heat treatment for Nimonic 105?

Four-step: (1) Solution at 1150 °C for 4 hrs, air cool; (2) 1065 °C for 16 hrs, air cool; (3) 980 °C for 16 hrs, air cool; (4) 795 °C for 16 hrs, air cool. Total cycle ~80–90 hrs. This produces dual-size gamma prime distribution maximizing creep-rupture strength. Simplifying the sequence will reduce properties.

Q9. Is Nimonic 105 weldable?

Extremely difficult to weld due to ~9% Al+Ti promoting strain-age cracking in the HAZ. Fusion welding is generally not recommended. When required, weld in solution-treated condition with minimal heat input (GTAW, near-matching filler), then full four-step heat treat. Resistance and EB welding preferred for limited applications.

Q10. What are the main applications of Nimonic 105?

HP and IP turbine blades, turbine discs, shafts, aerospace fasteners for 600–800 °C service, industrial gas turbine hot-section forged components. Historically used in Rolls-Royce Spey, Dart, and Tyne engines.

Q11. What is the typical price of Nimonic 105?

Round bar: USD 60–120/kg FOB Shanghai (2026). Forgings: USD 80–150/kg equivalent. Minimum orders 50–100 kg for bar. Lead time 6–10 weeks due to specialty melting and multi-step heat treatment.

Q12. What forms of Nimonic 105 are available?

Round bar 6–200 mm (solution-treated), forging stock and custom forgings per drawing, billets 150–350 mm, limited wire 0.5–5.0 mm, and limited sheet/plate up to 20 mm.

Contact Us for Nimonic 105

Hangbo Alloy Group provides mill-direct supply of Nimonic 105 bar, forging, billet, and wire to gas turbine manufacturers and aerospace OEMs worldwide. Our material is VIM+VAR melted, solution-treated, and fully certified per Rolls-Royce MSRR, GE, and customer OEM specifications. We can assist with grain size optimization for your specific creep-rupture requirements, heat treatment consulting, coating specification, and export documentation for aerospace-grade shipments.

For quotations, material certifications, or technical consultation, contact our sales team or call +86 13611656360. We typically respond within 10 minutes.

Need Nimonic 105 Material?

Request a quotation for Nimonic 105 bar, forging, or billet with OEM-spec certification. VIM+VAR melting, Rolls-Royce MSRR compliance, and creep-rupture testing available.